Open-access The effect of synthesis parameters on the catalytic synthesis of multiwalled carbon nanotubes using Fe-Co/CaCO3 catalysts

Fe-Co bimetallic catalysts supported on CaCO3 were prepared by a wet impregnation, a deposition-precipitation and a reverse micelle method. The sizes of the Fe and Co particles were not affected by the Fe and Co sources (nitrate, acetate) when the wet impregnation and deposition-precipitation methods were used. 'Clean' multi-walled carbon nanotubes (MWCNTs) were obtained from all three Fe-Co synthesis procedures under optimal reaction conditions. The CNTs produced gave yields ranging from 623 % to 1215 % in 1 h under the optimal conditions, with similar outer diameters (o.d.) of 20-30 nm and inner diameters (i.d.) ~10 nm. The Fe/Co catalyst formed in the wet impregnation method revealed that the yield, diameter and purity of the CNTs were influenced by the C2H2/N2 ratio, time and temperature. All the methods gave high-quality CNTs after short reaction times but the quality deteriorated as the synthesis time was increased from 5 to 360 min. Indeed, the most influential parameter in controlling CNT purity, length and o.d. was found to be the synthesis time. The as-synthesized CNTs were purified using a single-step mild acid treatment process (30 % HNO3), which readily removed the support and metal particles.

Carbon nanotubes; synthesis; bimetallic catalyst; iron; cobalt


RESEARCH ARTICLE

The effect of synthesis parameters on the catalytic synthesis of multiwalled carbon nanotubes using Fe-Co/CaCO3 catalysts

Sabelo D. MhlangaI, II; Kartick C. MondalI, II; Robin CarterI, II; Michael J. WitcombII, III; Neil J. CovilleI, II

IMolecular Sciences Institute and School of Chemistry, University of the Witwatersrand, Johannesburg, WITS 2050, South Africa
IIDST/NRF Centre of Excellence in Strong Materials, University of the Witwatersrand, Johannesburg, WITS 2050, South Africa
IIIMicroscopy and Microanalysis Unit, University of the Witwatersrand, Johannesburg, WITS 2050, South Africa

ABSTRACT

Fe-Co bimetallic catalysts supported on CaCO3 were prepared by a wet impregnation, a deposition-precipitation and a reverse micelle method. The sizes of the Fe and Co particles were not affected by the Fe and Co sources (nitrate, acetate) when the wet impregnation and deposition-precipitation methods were used. 'Clean' multi-walled carbon nanotubes (MWCNTs) were obtained from all three Fe-Co synthesis procedures under optimal reaction conditions. The CNTs produced gave yields ranging from 623 % to 1215 % in 1 h under the optimal conditions, with similar outer diameters (o.d.) of 20-30 nm and inner diameters (i.d.) ~10 nm. The Fe/Co catalyst formed in the wet impregnation method revealed that the yield, diameter and purity of the CNTs were influenced by the C2H2/N2 ratio, time and temperature. All the methods gave high-quality CNTs after short reaction times but the quality deteriorated as the synthesis time was increased from 5 to 360 min. Indeed, the most influential parameter in controlling CNT purity, length and o.d. was found to be the synthesis time. The as-synthesized CNTs were purified using a single-step mild acid treatment process (30 % HNO3), which readily removed the support and metal particles.

Keywords: Carbon nanotubes, synthesis, bimetallic catalyst, iron, cobalt

Full text available only in PDF format.

Acknowledgements

We gratefully acknowledge financial support from the National Research Foundation, Mellon Postgraduate Mentoring Scheme, the CSIR and the University of the Witwatersrand. We also thank Mr Rudolf Erasmus for his assistance with Raman spectral collection and analysis.

References

  • 1 S. Iijima, Nature, 1991, 354, 56-66.
  • 2 S. Iijima, Physica B, 2002, 323, 1-5.
  • 3 B.M. Endo, T. Hayashi, Y.A. Kim, M. Terrones and M.S. Dresselhaus, Phil. Trans. Roy. Soc. London, A, 2004, 362, 2223-2238.
  • 4 P. Ball, Made to Measure: New Materials for the 21st Century, Princeton University Press, Princeton, NJ, USA, 1997.
  • 5 M. Terrones, A. Jorio, M. Endo, Y.A. Kim, T. Hayashi, H. Terrones, J.-C. Charlier, G. Dresselhaus and M.S. Dresselhaus, Mater. Today, 2004, 7, 30-45.
  • 6 H. Zeng, L. Zhu, G. Hao and R. Sheng Carbon, 1998, 36, 259-261.
  • 7 Z.J. Shi, Y.F. Lian, X.H. Zhou, Z.N. Gu, Y. Zhang, S. Iijima, L. Zhou and K.T. Yue, Carbon, 1999, 37, 1449-1453.
  • 8 A. Thess, R. Lee, P. Nikolaev, H. Dai, P. Petit, J. Robert, C. Xu, Y.H. Lee, S.G. Kim, A.G. Rinzler, D.T. Colbert, G.E. Scuseria, D. Tombnek and J.E. Fischer, Science, 1996, 273, 483-487.
  • 9 D.C. Li, L. Dai, S. Huang, A.W.H. Mau and Z.L. Wang, Chem. Phys. Lett., 2000, 316, 349-355.
  • 10 V. Ivanov, J.B. Nagy, P. Lambin, A. Lucas, X.B. Zhang, X.F. Zhang, D. Bernaerts, G. Van Tendeloo, S. Amelinckx and J. Van Landuyt, Chem. Phys. Lett., 1994, 223, 329-335.
  • 11 R. Brukh and S.C. Mitra, Chem. Phys. Lett, 2006, 424, 126-132.
  • 12 K. Hernadi, A. Fonseca, J.B. Nagy, D. Bernaerts, J. Riga and A. Lucas, Synthetic Metals, 1996, 77, 31-34.
  • 13 K. Hernadi, Z. Kónya, A. Siska, J. Kiss, A. Oszkó, J.B. Nagy and I. Kiricsi, Mat. Chem. Phys., 2002, 77, 536-541.
  • 14 A.L. Balch and M.M. Olmstead, Chem. Rev., 1998, 98, 2123-2166.
  • 15 K. Hernadi, A. Fonseca, J.B. Nagy, A. Fudala, D. Baenaerts and A. Lucas, Zeolites, 1996, 17, 416-423.
  • 16 P. Francesco, Catal. Today, 1998, 41, 129-137.
  • 17 E. Couteau, K. Hernadi, J.W. Seo, L. Thiên-Nga, C. Mikó, R. Gaál and L. Forró, Chem. Phys. Lett., 2002, 378, 9-17.
  • 18 H. Kathyayini, N. Nagaraju, A. Fonseca and J.B. Nagy, J. Mol. Catal., 2004, 223, 129-136.
  • 19 M.C. Bahome, L.L. Jewell, D. Hildebrandt, D. Glasser and N.J. Coville, Appl. Catal. A: General, 2005, 287, 60-67.
  • 20 J. Cheng, X. Zhang, Z. Luo, F. Liu, Y. Ye, W. Yin, W. Liu andY. Han, Mat. Chem. Phys., 2006, 95, 5-11.
  • 21 A. Magrez, J.W Seo, C. Mikó, K. Hernádi and L. Forro, J. Phys. Chem. B, 2005, 109, 10087-10091.
  • 22 A. Magrez, J.W. Seo, VL. Kuznetsov and L. Forró, Angew. Chem. Int. Ed. Engl., 2007, 46, 441-444.
  • 23 P. Serp, M. Cossias and P. Kalck, Appl. Catal. A: General, 2003, 253, 337-358.
  • 24 Z. Yu, D. Chen, B. Totdal and A. Holmen, Catal. Today, 2005, 100, 261-267.
  • 25 A.-C. Dupuis, Prog. Mat. Sci., 2005, 50, 17-20.
  • 26 W. Qian, T. Liu, Z. Wang, H. Yu, Z. Li, F. Wei and G. Luo, Carbon, 2003, 41, 2487-2493.
  • 27 B. Louis, G. Gulino, R. Vieira, J. Amadou, T. Dintzer, S. Galvagno, G. Centi, M.J. Ledoux and C. Pham-Huu, Catal. Today, 2005, 102-103, 23-28.
  • 28 G. Che, B.B. Lakshmi, C.R. Martin and E.R. Fisher, Chem. Mater., 1998, 10, 260-267.
  • 29 E. Dervishi, Z. Li, A.R. Biris, D. Lupu, S. Trigwell and A.S. Biris, Chem. Mater., 2007, 19, 179-184.
  • 30 T.C. Schmitt, A.S. Biris, D.W. Miller, A.R. Biris, D. Lupu, S. Trigwell and Z.U. Rahman, Carbon, 2006, 44, 2032-2038.
  • 31 C.H. See and A.T. Harris, Particle Tech. Fluidization, 2008, 54, 657-664.
  • 32 (a) M. Boutonnet, J. Kizling and P. Stenius, Colloids and Surfaces, 1982, 5, 209-225;
  • (b) E.E. Carpenter, J. Magnetism Magnetic Mater., 2001, 225, 17-20;
  • (c) C.T. Seip and C.J. O'Connor, Nanostr. Mater., 1999, 12, 183-186;
  • (d) I. Ban, M. Drofenik and D. Makovec, J. Magnetism Magnetic Mater., 2006, 307, 250-256;
  • (e) Y. Lee, J. Lee, C.J. Bae, J.-G. Park, H.-J. Noh, J.-H. Park and T. Hyeon, Adv. Funct. Mater., 2005, 15, 503-509;
  • (f) V. Pillai, P. Kumar, M.S. Multani and D.O. Shah, Colloids and Surfaces A: Physicochem. Eng. Aspects, 1993, 80, 69-75.
  • 33 M. Escober, M.S. Moreno, R.J. Candal, M.C. Marchi, A. Caso, P.I. Polosecki. G.H. Rubiolo and S. Goyanes, Appl. Surf. Sci., 2007, 254, 251-256.
  • 34 (a) A. Zhang, C. Li, S. Bao and Q. Xu, Microp. Mesop. Mater., 1999, 29, 383-388;
  • (b) J.-B. Park, G.-S. Choi, Y.-S. Cho, S.-Y. Hong, D. Kim, S.-Y Choi, J.-H. Lee and K.-I. Cho, J. Cryst. Growth, 2002, 244, 211-217;
  • (c) C. Emmenegger, P. Mauron, A. Züttel, C. Nützenadel, A. Schneuwly, R. Gallay and L. Schlapbach, Appl. Surf. Sci., 2000, 162-163, 452-456.
  • 35 S.D. Mhlanga and N.J. Coville, Diam. Rel. Mater., 2008, 17, 1489-1493.
  • 36 A. Jorio, M.A. Pimenta, A.G.S. Filho, R. Saito, G. Dresselhaus and M.S. Dresselhaus, New J. Phys., 2003, 5, 139.1-139.17.
  • 37 Z.L. Wang and Z.C. Kang, J. Phys. Chem., 1996, 100, 5163-5165.
  • 38 V.G. Pol, M. Motiei, A. Gedanken, J. Calderon-Moreno and M. Yoshimura, Carbon, 2004, 42, 111-116.
  • 39 http://www.carbonblack.jp/en^cb/youto.html#top. Accessed 1 June 2007.
    » http://www.carbonblack.jp/en^cb/youto.html#top
  • 40 M. Monthioux, H. Allouche and R.L. Jacobsen, Carbon, 2006, 44, 3183-3194.

Received 17 December 2007
Revised 22 December 2008
Accepted 7 February 2009

* To whom correspondence should be addressed. E-mail:

Correspondence

neil.coville@wits.ac.za.

Publication Dates

  • Publication in this collection
    16 July 2015
  • Date of issue

History

  • Received
    17 Dec 2007
  • Reviewed
    22 Dec 2008
  • Accepted
    07 Feb 2009
location_on
The South African Chemical Institute The South African Journal of Chemistry, University of the Witwatersrand, The Secretary - Laila Smith, School of Chemistry, Private Bag X3, Braamfontein, Johannesburg, ZA, 2050, Tel:+27 11 717 6705, 061 282 3477 - E-mail: editorsajchem@saci.co.za
rss_feed Stay informed of issues for this journal through your RSS reader
Go to top