Abstract
Wet gases are typically produced and transported through carbon steel pipeline systems. The combination of corrosive gases and transportation conditions creates highly aggressive environments, often leading to recurring incidents of pipeline corrosion failure. This study investigated the corrosion rate on the internal upper surface of the X65 carbon steel pipeline under static conditions, where gas flow is dominated by natural convection. To replicate realistic field conditions, a novel apparatus was designed to measure condensation rates, water droplet lifespan, and top-of-line corrosion (TLC) rates across a wide range of steel surfaces and gas temperatures. Surface morphology was characterized using SEM imaging to evaluate the corrosion morphology and identify the types of corrosion deposits. The findings reveal that when the surface temperature is at or below 30°C, TLC is primarily governed by the water condensation rate and surface temperature. However, at surface temperatures above 30°C, the condensation rate becomes the dominant controlling parameter. In the top of the line (TOL) scenario, the lifetime of the condensed water droplet plays a critical role in determining the corrosion rate. The results further demonstrate that the droplet lifespan affects the formation and precipitation of the FeCO3 film, which in turn influences corrosion behavior.
top of line corrosion; gas temperature; steel temperature; water condensation rate
INTRODUCTION
Crude oil and natural gas are typically transported through carbon steel pipelines, and this stage in oil and gas production presents significant corrosion risks. The produced oil is typically unprocessed and contains a combination of gas, brine, and solids. The presence of various dissolved gases, such as carbon dioxide (CO2), hydrogen sulphide (H2S), and organic acids (e.g., acetic and formic acid), in combination with brine, can lead to severe corrosion problems at the internal surfaces of carbon steel pipelines.1
One specific form of corrosion associated with wet gas production is known as Top-of-Line Corrosion (TLC). TLC was first discovered in the 1960s and became widely recognized in the context of wet gas transportation, particularly when significant heat exchange occurs between the transported gas and the adjacent environment. If the flow regime of multiphase fluids (gas/liquid) is stratified, the saturated water vapor can condense at the inner wall of the pipeline due to the temperature differences between the outside environment and the produced fluid.12, H2S, and corrosive species such as organic acids, forming a corrosive chemical solution with properties significantly different from those flowing at the bottom of the pipeline.
Figure 1 clearly distinguishes between the two primary corrosion mechanisms in wet gas systems: Top-of-the-Line (TOL) corrosion results from the condensation of water vapor on the inner upper surface of the pipeline due to temperature gradients between the gas phase and the pipeline wall. The resulting droplets create localized corrosive environments unique to the gas-phase condensate. Bottom-of-the-Line (BOL) corrosion, by contrast, occurs in the stratified liquid layer at the bottom of the pipe, where the aqueous phase is in continuous contact with the steel surface. The chemistry of this bulk liquid can differ significantly from the condensate droplets at the top.
The condensed liquid in the pipeline has a pH value ranging from 3 to 4 due to the absence of minerals and bases in the solution.21
Since the first reported case in 1960 in France,31,2,4-10 Most of these models consider the influences of water condensation rate (WCR) and gas temperature (Tg); however, when calculating WCR, they primarily account for the surface temperature (Ts) through heat transfer via the pipeline walls. These factors govern the dissolution process of the steel surface and determine whether the condensed water is saturated with iron carbonate (FeCOj). This saturation facilitates and enhances the process of iron carbonate precipitation onto the steel surface, forming a protective layer of iron carbonate that can hinder further steel dissolution.1, 4s, Tg, and WCR.1,4
Although previous studies have extensively investigated the mechanisms oftop-of-line corrosion (TLC), their focus predominantly revolved around specific variables like the water condensation rate (WCR) and the influence of gas temperatures (Tg) on corrosion rates. These studies have laid significant groundwork, but often relied on assumptions or limited experimental conditions.4, 11-13
This study aims to address these gaps by employing a novel experimental setup and conducting a comprehensive analysis. Isolating the most influential factors remains one of the most challenging steps in understanding the TLC mechanism. This research presents a TLC setup designed to simultaneously measure the actual surface and gas temperature, collect the condensed water, and determine the water condensation rate. This setup allowed for a clear distinction between the individual impacts of two interrelated parameters, water condensation rate (WCR) and surface temperature (Ts), on the TLC. Additionally, the thermodynamics and kinetics of FeCO3 scale formation at the top-of-line are examined using SEM imaging and X-ray diffraction (XRD).
NOVELTY IN EXPERIMENTAL SETUPSinger et al. introduced a setup that explored TLC under sour conditions using carbon dioxide and hydrogen sulfide environments.1 s) and water condensation rate (WCR). In contrast, the innovative design developed here measures these parameters concurrently, providing a more comprehensive view of their synergistic effects on TLC. This dual-factor approach enables a more precise understanding of how temperature gradients influence both condensation dynamics and corrosion mechanisms.
Islam et al. primarily focused on condensation corrosion at moderate surface temperatures and its relationship with FeCO3 precipitation kinetics.4s values, where unique phenomena such as the decoupling of WCR influence at Ts > 30°C were observed.
EXPERIMENTAL METHODS
Experimental TLC Test Cells
Experiments at atmospheric pressure were conducted using glass cells, each cell containing two X65 carbon steel coupons. Figure 2 illustrates a photograph of the TLC cell employed in the experiments.
The standard elemental composition of the X65 samples is summarized in Table 1. Each sample was machined into a cylindrical form with a diameter of 25 mm and a thickness of 10 mm. A central hole, 2 mm in diameter and 9 mm in depth was drilled into each sample, leaving 1 mm from the bottom surface of the sample to accommodate a temperature probe for the measurement of the surface temperature (Ts). During the test, the X65 coupons were flush-mounted into the lids of the glass cells, and oil was dropped into the hole to ensure consistent and stable surface temperature measurements.
To control the water condensation process, a 10 mm diameter spiral copper coil was placed around the holder, through which water was circulated to cool the sample and achieve the desired surface temperature (Ts). The target gas temperature (Tg) was achieved by heating the bottom solution using a hot plate. This design created an in-situ condensation process that mimics field pipeline conditions.
The aqueous solution consists of CO2-saturated distilled water, which had been purged with CO2 gas for at least 12 hours prior to the start of each experiment to ensure minimum oxygen content in the water. Additionally, during the experiments, CO2 gas was continuously bubbled into the solution to maintain complete saturation.
For WCR and pH measurements of the condensate, condensed water was collected by a small funnel installed beneath the test sample and immediately transferred to a sealed, CO2-saturated collection container. WCR measurements were carried out twice daily throughout the test period, which lasted 168 hours.
The mass loss technique for measuring the rate of corrosion was employed in this study due to difficulties with performing electrochemical corrosion measurements under top-of-line conditions over extended periods. This method imposes a limitation because it provides integrated results, unlike electrochemical tests, which give real-time corrosion rates. However, the transient behavior was investigated by regular measurements taken after 24, 48, 72, 96, 120, 144, and 168 hours.
To ensure the accuracy and reliability of the results, the experiments were repeated at least three times. Error bars represent the minimum and maximum corrosion rate values under each test condition are shown in the graphs. The test matrix for the experiments is presented in Table 2.
Experimental Measurements of Condensation and Corrosion Rates
Throughout the pre-test preparations, the exposed surfaces of samples were polished using grit sandpaper up to 1200 grit, then washed with isopropanol solution and dried with a heat gun. After that, the side and the upper face of each sample were coated carefully with a thin layer of protective lacquer.
The samples were then wet-grounded and weighed using a high-precision digital scale with a resolution of 0.05 mg to measure their initial mass (m1) before being mounted into the lid. The required inner surface temperature was achieved and maintained using a cooling chamber. To accomplish this, it was possible to control the temperature at which cold water circulates through copper coils around the sample. The water condensation rates were calculated using the following equation:
where, WCR = water condensation rate, (g/m2W= condensed water volume, (ml); pW = water density, (g/cm3c = duration time over which the condensate is collected, (s); St = sample surface area, (m2
Following each corrosion rate measurement, samples were taken and rinsed with distilled water, then ethanol, and gently dried using an air gun. The samples were then weighed to record their post-exposure mass (m214 2
where, CR is the corrosion rate, mm/y; (m1 - m2) is the mass loss, grams; pFe is the carbon steel density = 7.85 g/cm32
EXPERIMENTAL RESULTS AND ANALYSISThe results are subdivided into two main categories: water condensation rate and weight loss corrosion results.
Water Condensation Rates
Figure 3 shows the in-situ average WCR measurements across a range of gas (Tg) and steel surface (Ts) temperatures over a test period of 168 hours.
According to the results of these experiments, the maximum temperature difference between bulk gas and the steel surface of 45°C was observed when Tg = 60°C and Ts = 15°C, resulting in a WCR of 1.70 mL/m22g is 30°C and Ts is 25°C.
It is clear from the WCR measurements that the temperature difference between the bulk gas and the steel temperature is a critical factor influencing the rate of condensation. This relationship can be attributed to the fact that when temperatures are increased, a higher rate of condensation is also achieved due to an increase in humidity, which enhances heat and mass transfer, as described by Nusselt's theory of condensation.2,15,16
Average Corrosion Rates
The two main parameters, steel surface temperature and water condensation rate are considered the primary factors controlling the corrosion threat on the top surface of the pipeline.13,17 Consequently, these parameters were systematically varied to assess their influence on the average corrosion rate for X65 carbon steel over time.
Surface Temperature Effect
Across all corrosion experiments, two notable trends were observed. First, the average corrosion rate significantly increased over time. Second, after an initial period of stability, the values of the average corrosion rate exhibited a gradual decline. The results of both scenarios are presented in Figure 4.
When Tg is 40°C, the average corrosion rate increases with time at Ts of 15 and 30°C, as shown in Figure 4 (a). This behavior is attributed to the formation of an iron carbide layer (Fe3C), a corrosion product which is commonly observed in corrosion products in the CO2 corrosion process of low alloy carbon steels,18Figure 5 and Figure 6 (a).
Fe3C is often left on the metal surface after a corrosion process because it is more difficult to dissolve in an aqueous solution than the ferrite phase (α-Fe).18s = 38°C and Tg = 40°C, where the corrosion rate began to decline after 96 hours. A similar trend was observed at Tg was 50°C, as illustrated in Figure 4 (b), although a more pronounced increase in the average corrosion rate was noted at Ts = 15°C and 30°C, followed by a reduction at Ts = 38°C.
It is well known that Fe3C is an electrochemical conductor and acts as a cathodic site when hydrogen ions are reduced. The iron carbide and ferrite phases affect the steel microstructure, where iron carbide can accelerate corrosion, and ferrite is subject to dissolution, resulting in an eroded surface. A galvanic cell is formed between the corroded ferrite, which acts as the anode, and iron carbide, which acts as a cathode. As the corrosion process continues, more Fe3C forms, leading to an enhancement in cathodic reactions and, consequently, higher average corrosion rates.19-21
All experiments were classified as either FeCO3 film-forming or non-forming based on ex-situ analysis of sample surfaces and corrosion rate results at the end of the 168-hour test period.
The results indicate that protective films formed on sample surfaces when certain conditions were met during the experiments. Representative SEM images illustrating the visual appearance of the surface with and without the FeCO3 film are presented in Figure 6. Additionally, the XRD pattern shown in Figure 6 (c) confirms that the corrosion product observed in Figure 6(b) is FeCO3.
WCR Effect
The influence of Ts and WCR on top-of-line corrosion (TLC) is presented in Figure 7. The corrosion rate is expected to increase significantly with the WCR due to the more frequent renewal of water droplets at higher condensation rates.
A significant increase in WCR, from 0.31 to 1.71 mL/m2
At higher surface temperatures, such as 30°C and 38°C, WCR had a greater impact on the corrosion rate. For instance, an increase in WCR from 0.29 to 1.34 mL/m22
Based on these obtained results and the previous observation, it can be deduced that under low-temperature conditions, the corrosion rate is essentially dependent upon steel temperature and is relatively insensitive to the water condensation rate (WCR). This behavior is due to the lower rate of iron dissolution at reduced surface temperatures, resulting in an extremely low concentration of Fe2
Under these conditions, the corrosion reaction is controlled by the steel temperature rather than the gas temperature. Additionally, at low WCRs, droplets can remain attached to the top inner surface for extended periods, allowing conditions to become favourable for the formation of iron carbonate scales within droplets. Therefore, the combination of a high surface temperature and prolonged droplet lifetime promotes the formation of a protective iron carbonate film on the surface.
CONCLUSIONS
In this study, water condensation and inner surface temperature were systematically varied over time to assess their effect on the top-of-the-line corrosion of carbon steel in a CO2_rich environment. Based on the experimental findings, the following conclusions can be drawn:
• A critical temperature threshold of the pipeline surface (Ts > 30°C) was identified, above which corrosion rate is predominantly governed by surface temperature and WCR. Whereas, below this temperature, WCR has minimal impact on TLC rates
• At lower surface temperatures, no substantial differences were noted in the corrosion rates, even though WCRs increased. Whereas, at high sample surface temperature, increasing WCR significantly accelerates corrosion.
• Droplet lifetime plays a critical role in FeCO3 film formation under TOL conditions. Short-lived droplets may not allow film formation even at high supersaturation.
• FeCO3 film formation and precipitation behavior differ between TOL and BOL conditions. While high supersaturation typically promotes film formation at BOL, TOL conditions require sustained droplet presence on the surface.
These findings highlight the complex interdependence of Ts, WCR, and droplet behavior in governing TLC mechanisms and have practical implications for corrosion prediction and mitigation in wet gas pipelines.
AUTHOR CONTRIBUTIONSThe author confirms sole responsibility for all aspects of the study, including conceptualization, methodology, investigation, writing, and final review and editing.
CONFLICT OF INTERESTThe author declares that there are no conflicts of interest regarding the publication of this manuscript.
DECLARATION OF GENERATIVE AI AND AI-ASSISTED TECHNOLOGIES
Not applicable.
ORCID IDKhalid A. Mohammed: https://orcid.org/0000-0002-0207-3479
ACKNOWLEDGMENTS
The author is grateful to the Petroleum and Gas Engineering Department and the University of Thi-Qar for their financial and scientific support.
REFERENCES
-
1. Singer M, Al-Khamis J, Nešić S. Experimental study of sour top-of-the-line corrosion using a novel experimental setup. Corrosion. 2013;69(6):624-638. https://doi.org/10.5006/0738E
» https://doi.org/10.5006/0738E -
2. Mohammed KA. Experimental and theoretical investigation of top-of-the-line corrosion in CO2 gas and oil environments. PhD thesis, University of Leeds; 2018. https://etheses.whiterose.ac.uk/id/eprint/20479/
» https://etheses.whiterose.ac.uk/id/eprint/20479/ -
3. Jenkins A, Gilbert I. Development of a Top-of-Line Corrosion Inhibitor and a Top-of-Line Corrosion Test Method. Proceedings of the CORROSION 2012. CORROSION 2012. Salt Lake City, Utah, USA; March 11-14, 2012. pp 1-12). AMPP. https://doi.org/10.5006/C2012-01275
» https://doi.org/10.5006/C2012-01275 -
4. Islam MM, Pojtanabuntoeng T, Gubner R. Condensation corrosion of carbon steel at low to moderate surface temperature and iron carbonate precipitation kinetics. Corros Sci. 2016;111:139-150. https://doi.org/10.1016/j.corsci.2016.05.006
» https://doi.org/10.1016/j.corsci.2016.05.006 -
5. Méndez C, Singer M, Camacho A, Hernández S, Nesic S, Gunaltun Y, Joosten M, Sun Y, Gabbetta P. Effect of acetic acid, pH and MEG on the CO2 top of the line corrosion. Corrosion. 2005;2005:1-27. https://doi.org/10.5006/C2005-05278
» https://doi.org/10.5006/C2005-05278 -
6. Egab K, Mohammed KA, Okab AK, Oudah S. Numerical study of condensation heat transfer and droplet dynamics on different wetting surfaces of gas transportation pipelines. IOP Conference Series: Materials Science and Engineering, Volume 928, 2nd International Scientific Conference of Al-Ayen University (ISCAU-2020) 15-16 July 2020, Thi-Qar, Iraq. Article 022105. https://doi.org/10.1088/1757-899X/928/2/022105
» https://doi.org/10.1088/1757-899X/928/2/022105 -
7. Neshati J, Saremi M, Mashhadi G. A new approach in top-of-line corrosion studies in CO2/H2S environment. Corros Eng Sci Technol. 2023;58(8):723-733. https://doi.org/10.1080/1478422X.2023.2250156
» https://doi.org/10.1080/1478422X.2023.2250156 -
8. Stack MM, Abdulrahman GH. Mapping erosion-corrosion of carbon steel in oil-water solutions: Effects of velocity and applied potential. Wear. 2012;274-275:401-413. https://doi.org/10.1016/j.wear.2011.10.008
» https://doi.org/10.1016/j.wear.2011.10.008 -
9. Albrahim I, Al-Abbas F, Costa RS, Debruyn H, Al-Saif O. Probe into water chemistry effects on internal corrosion risk for sour gas pipelines. J Pipeline Syst Eng Pract. 2024;15(2):04024002. https://doi.org/10.1061/JPSEA2.PSENG-1447
» https://doi.org/10.1061/JPSEA2.PSENG-1447 -
10. Al-Moubaraki AH, Obot I. Top of the line corrosion: causes, mechanisms, and mitigation using corrosion inhibitors. Arab J Chem. 2021;14(5):103116. https://doi.org/10.1016/j.arabjc.2021.103116
» https://doi.org/10.1016/j.arabjc.2021.103116 -
11. Yaakob N, Singer M, Young D. Top of the line corrosion behavior in highly sour environments: effect of the gas/steel temperature. Proceedings of the CORROSION 2014. CORROSION 2014. San Antonio, Texas, USA; March 9-13, 2014. AMPP. pp 1-10. https://doi.org/10.5006/C2014-3807
» https://doi.org/10.5006/C2014-3807 -
12. Singer M, Hinkson D, Zhang Z, Wang H, Nesic S. CO2 top-of-the-line corrosion in the presence of acetic acid: a parametric study. Corrosion. 2013;69(7):719-735. https://doi.org/10.5006/0737.
» https://doi.org/10.5006/0737 -
13. Singer M, Nesic S, Gunaltun Y. Top of the line corrosion in presence of acetic acid and carbon dioxide. Proceedings of the CORROSION 2004. CORROSION 2004. New Orleans, Louisiana, USA; March 27-April 1, 2004. AMPP. pp. 1-20. https://doi.org/10.5006/C2004-04377
» https://doi.org/10.5006/C2004-04377 -
14. Metals ACG-Co. Standard practice for preparing, cleaning, and evaluating corrosion test specimens. West Conshohocken: ASTM International; 2011. https://doi.org/10.1520/G0001-03R17E01
» https://doi.org/10.1520/G0001-03R17E01 -
15. Rose JW. Enhanced condensation heat transfer. JSME Int. J. Ser. B. 2006; 49(3):626-635. https://doi.org/10.1299/jsmeb.49.626
» https://doi.org/10.1299/jsmeb.49.626 -
16. Stephan K, Green CV. Heat transfer in condensation and boiling. Springer; 1992. https://doi.org/10.1007/978-3-642-52457-8
» https://doi.org/10.1007/978-3-642-52457-8 -
17. Nyborg R, Dugstad A. Top of line corrosion and water condensation rates in wet gas pipelines. Proceedings of the CORROSION 2007. CORROSION 2007. Nashville, Tennessee, USA; March 11-15, 2007. AMPP. pp 1-10. https://doi.org/10.5006/C2007-07555
» https://doi.org/10.5006/C2007-07555 - 18. Vitse F. Experimental and theoretical study of the phenomena of corrosion by carbon dioxide under dewing conditions at the top of a horizontal pipeline in the presence of non-condensable gas. PhD Thesis, Ohio University, USA; 2002.
-
19. López DA, Simison S, De Sanchez S. The influence of steel microstructure on CO 2 corrosion. EIS studies on the inhibition efficiency of benzimidazole. Electrochim Acta. 2003;48(7):845-854. https://doi.org/10.1016/S0013-4686(02)00776-4
» https://doi.org/10.1016/S0013-4686(02)00776-4 -
20. Eliyan FF, Alfantazi A. On the theory of CO 2 corrosion reactions-Investigating their interrelation with the corrosion products and API-X100 steel microstructure. Corros Sci. 2014;85:380-393. https://doi.org/10.1016/j.corsci.2014.04.055
» https://doi.org/10.1016/j.corsci.2014.04.055 -
21. Gao M, Pang X, Gao K. The growth mechanism of CO2 corrosion product films. Corros Sci. 2011;53(2):557-568. https://doi.0rg/1O.1O16/j.corsci.2010.09.060
» https://doi.0rg/1O.1O16/j.corsci.2010.09.060
Revised 16 July 2025